Measuring Residual Stresses: A Comparison of Direct vs. Indirect Methods
How to extend the service life of your components
Residual stresses are invisible but crucial: They influence how long a component lasts, how resistant it is to fatigue, and whether it will fail during operation. Especially in the automotive, aerospace, and medical technology industries, the targeted measurement of residual stresses can make the difference between success and costly failure. But how can these stresses inside the material be determined in the first place? Two methods are in focus: the rapid borehole method for practical use and high-precision X-ray diffraction as the gold standard. This article explains how both methods work, what advantages and disadvantages they offer—and when each approach is worth the effort.
Direkte vs. indirekte Eigenspannungsmessung: Welche Methode passt zu Ihrem Bauteil?
According to Hooke’s law, there is a very simple and linear relationship between stress and strain. Residual stresses can therefore also be expressed in terms of the strain in the metal microstructure. In residual stress measurement, the strain of the microstructure is essentially measured and converted into stress accordingly.
There are two basic methods for determining this strain. The strain in the microstructure can be measured either directly or indirectly. Direct measurement utilizes the effect of X-ray diffraction, which allows the lattice spacing to be measured (Figure 1).
In indirect measurement, on the other hand, one takes advantage of the fact that a component must always be in equilibrium with respect to its residual stress state. This means that the sum of all stresses must always equal 0.
∑ σ = 0
However, this also means that if the state of equilibrium is disturbed, it must be restored. If material is removed in a controlled manner, the material responds by deforming. This deformation can be measured and converted into a stress value.
Borehole Method: Rapid Residual Stress Measurement with Strain Gauges - Advantages and Limitations
A commonly used indirect measurement method is the strain gauge borehole method (Figure 2). It is an indirect method for measuring residual stress. In this method, a borehole that is as cylindrical as possible is drilled into the surface of the component at defined depth intervals. In most cases, the borehole has a diameter of approximately 0.8–3 mm and a depth of about 1.5 times the diameter.
Removing material from the surface causes it to deform. This deformation can be measured using a strain gauge rosette. Three strain gauges measure the deformation at 0°, 45°, and 90°.
By drilling and measuring in stages, a complete depth profile can be recorded in a relatively short time. The measurement is therefore performed quickly, although here too, the greatest effort lies in preparing the hole and the strain gauge. Experienced measurement technicians require only a few hours to complete a measurement.
A disadvantage, however, is that the measurement has a somewhat higher measurement uncertainty. It is also not possible to determine the surface residual stresses.
Due to the sensitivity of the strain gauge, the first measurement point must be located at a certain distance (approximately 35–50 µm) from the surface.
Advantages:
| Limitations:
|
Röntgendiffraktometrie: Präzise, aber aufwändig – Wann lohnt sich der Goldstandard?
Significantly more complex in terms of equipment, but also more accurate, is residual stress measurement using X-ray diffraction (Figure 3). This method utilizes the principle of X-ray diffraction.
This measurement method is much more time-consuming than drilling a small hole. The specimen is irradiated with a directed X-ray beam for several minutes (usually 20 minutes or more). This beam is reflected by the microstructure. According to Bragg’s law, a change in the lattice spacing causes a phase shift in the beam, which can be measured (Figure 4).
n ⋅ λ = 2dhkl ⋅ sin θB
In addition to measuring residual stress, X-ray diffraction can also be used for texture analysis or phase analysis. In phase analysis, a complete histogram (intensity profile) is evaluated, in which the incident angle (diffraction angle 2qB) is varied over a wide range. In residual stress measurement, the measurement is performed at only one peak of this profile. This means that a “fixed” diffraction angle is defined.
During the measurement, the beam is then passed through this defined angle once. The most commonly used evaluation method is the sin2y method.
The X-ray beam does not have sufficient energy to penetrate deep into the surface. Depending on the material, the depth of information for the measurement is a few micrometers (approximately 3 µm for steels). This means that a residual stress measurement therefore always provides information only from the “surface.” To obtain a depth profile, the surface must be removed in stages. This is usually done by electrochemical polishing. This process introduces virtually no new residual stresses. Due to the sufficiently large ratio of the removed surface area to the depth, it is assumed that no deformation occurs (acceptable simplification).
Furthermore, the measurement is direction-dependent. While the borehole method using a strain gauge allows for a single measurement in three directions, X-ray diffractometry requires the measurement to be repeated three times, with the specimen rotated each time. In most cases, the 45° direction is neglected, which means that the complete stress tensor cannot be determined unless the other two directions happen to correspond to the principal stresses.
Such a direct in-situ stress measurement is therefore much more time-consuming. A depth profile measured in two directions requires approximately 1–1.5 days of measurement time. In addition, much more expensive measurement equipment is required, and the technicians must possess much higher qualifications.
Despite all these drawbacks, residual stress measurement using X-ray diffraction remains the gold standard for residual stress measurement. It provides a highly accurate result with a precision of up to ±10 MPa (under optimal conditions). By comparison, the borehole method typically has a precision of ±100 MPa.
Advantages:
| Effort:
|
Measuring residual stresses in a targeted manner is the first step toward extending the Service life of your components. Whether you choose the borehole method or X-ray diffraction—the choice of method depends on your requirements. Would you like to learn more about how you can not only measure residual stresses but also introduce them specifically into your components? Then contact our experts or read our blog post on Deep Rolling.
Sources:
| [1] | Breidenstein, B., Surface and Edge Zone Properties of Highly Loaded Components. Habilitation thesis, Leibniz University Hannover, 2011 |
Frequently Asked Questions About Residual Stress Measurement
Which method is faster: the borehole method or X-ray diffractometry?
The borehole method delivers results in a few hours, while X-ray diffractometry takes 1–1.5 days.
Can I measure surface residual stresses using the borehole method?
No, the first measurement point is located approximately 35–50 µm below the surface.
For which industries is X-ray diffractometry particularly suitable?
Primarily in the aerospace and medical technology industries, where the highest accuracy is required.